| Usually
caused by |
Cured
by |
|
Flask being
heated too rapidly during de-wax.
|
Do not exceed
150oC during de-wax. Wax will boil and erode
investment surface.
|
|
Flasks
overheated during burnout.
|
Ensure
maximum burnout temperature does not exceed 740oC
|
|
Flasks
put in furnace too soon after investing.
|
Leave
flasks undisturbed for a minimum of one hour before de-wax.
|