Home Next Back

     Other flashing or finning 
 
Usually caused by Cured by
Work cycle too long. Investment beginning to set while still under vacuum. Ensuring the work cycle is not too long and slurry temperature is 20 - 22ºC. 
Disturbing the flasks too soon. Leave the flasks for at least one hour.
Heating too quickly during de-wax. Do not exceed 150ºC during de-waxing.
Moulds allowed to dry out before burnout. If not burning out the same day, keep moulds wet by covering with wet sacking or plastic sheets.
 
  Casting problems
  Wax pattern problems
  Mould rubber problems
Mixing guide
De-wax and  burnout cycles
Sitemap